June Perry on fri 19 jan 07


Here's a recipe for a beautiful matt black. I used it years ago in cone 10
reduction. It has the most wonderful finish - more of semi matt leaning to satin
rather than dry.

J.BOBBS MATT BLACK 10 REDUCTION OXIDATION

POTASH FELDSPAR 5584.8
WHITING 568.9
CHINA CLAY 1526.4

Total 7680.1

ADD: COBALT OXIDE 221.76, IRON OXIDE 253.5

Regards,
June
http://shambhalapottery.blogspot.com/
http://www.angelfire.com/art2/shambhalapottery