search  current discussion  categories  glazes - cone 4-7 

glaze test for white satin mat, cone 6, ox.

updated wed 10 may 06

 

Alisa Liskin Clausen on tue 9 may 06


Glaze test for White Satin Mat, cone 6, ox.




Source: Clayart, Kathy Rhoades

Credited to:



Fired on mid fire white stoneware.



Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 1 hour
Shut off kiln



Recipe:

31.6 Gerstely Borate subbed local high boron frit

13. 95 Talc

19.80 Kona F-4 Feldspar subbed Forshammer Feldspar

4.98 EPK

29.64 Silica



ADD

5.11 Zirocpax

1.99 Bentonite





Note: All raw materials are measured up or down to the nearest half
decimal. Colorants or additives to a 100 gram batch are measured in percent
to the 100 gram batch.



Results:

Mat, white glaze. Not well melted on thinner areas, with small bubbles.
Thicker areas has smooth and slightly pebbled textures.



Regards from Alisa in Denmark