glaze test for rutile mat, cone 6, ox. jayne shatz article

updated wed 10 may 06


Alisa Liskin Clausen on tue 9 may 06

Glaze test for Rutile Mat, cone 6, ox. Jayne Shatz article

Source: CM September 2006, Jayne Shatz article

Credited to:

Fired on mid fire white stoneware.

Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 1 hour
Shut off kiln


20 Whiting

56 Neph. Syenite

18 Kaolin

6 Silica


7 Rutile

9 Zinc. Ox.

Note: All raw materials are measured up or down to the nearest half
decimal. Colorants or additives to a 100 gram batch are measured in percent
to the 100 gram batch.


Mat, yellowish cream color, slight grey streaking overall.

Surface is varied with lighter cream crystals to greyish undertones where
glaze streaks.

Regards from Alisa in Denmark