search  current discussion  categories  glazes - cone 4-7 

glaze test for pam' frost, cone 6, ox.

updated wed 10 may 06


Alisa Liskin Clausen on tue 9 may 06

Glaze test for Pam's Frost, cone 6, ox.

Source: Clayart

Credited to: Pam Cressell

Fired on mid fire white stoneware.

Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 1 hour
Shut off kiln


21.4 Whiting

2.5 Zinc Ox.

15.4 Neph. Syenite

19.5 EPK

34.2 Silica

7.0 Spodumene


2.6 Tin Oxide

Note: All raw materials are measured up or down to the nearest half
decimal. Colorants or additives to a 100 gram batch are measured in percent
to the 100 gram batch.


Gloss, transparent cream white.