glaze test for noah's port, cone 6, oxidation

updated wed 10 may 06


Alisa Liskin Clausen on tue 9 may 06

Glaze test for Noah's Port, cone 6, oxidation

Source: Clayart

Credited to: Lili Krakowski

Fired on mid fire white stoneware.

Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 1 hour
Shut off kiln


60 Redart clay

20 Nepheline Syenite

10 Dolomite

20 Frit 3135 used local high Boron Frit



115 gr.

Note: All raw materials are measured up or down to the nearest half
decimal. Colorants or additives to a 100 gram batch are measured in percent
to the 100 gram batch.


Gloss glaze, dark brown to black ground under an overall varieagated rust
brown and green fur shell.

Regards from Alisa in Denmark