wirt shino recipe enclosed

updated wed 9 nov 05

 

June Perry on tue 8 nov 05


Here's a recipe for Wirt Shino

#1230 VIRGINIA WIRT SHINO C10 REDUCTION

KONA F4 SODASPAR 2408.8
SPODUMENE 2560.2
EDGAR PLASTIC KAOLIN 961.2
SODA ASH 349.6
TOTAL: 6279.8

Regards,
June