search  current discussion  categories  glazes - misc 

orange recipe from files

updated wed 2 nov 05

 

Lesley Alexander on tue 1 nov 05


Found this in my Clayart collection Lesley:

This cone 10 matt reduction orange is a staple at Florida Atlantic
University. It is
especially good in combination with ash glazes on, say the top 1/4, and matt
orange below.Has lots of motion & breaks - best on clay with some iron
content.

Custer Spar 52
EPK 25
Whiting 25
Talc 4
R.I.O. 6
Bone ash 4
Rutile 5