search  current discussion  categories  kilns & firing - wood 

woodfire-wading info?

updated mon 31 oct 05

 

Gary Georger on sat 29 oct 05


For an anagana/cofffin woodfire we've been using a
50/50 or so mix of EPK and alumina hydrate ..but am
interseted in not so white/bald wading marks so I'm
going to experiment with adding sawdust,coffee,rice,
oats sand,grog ....anyone have recipe or guidelines
for wading and proportions?
much appriecated
Gary

http://www.washingtonpotters.org
http://www.gallery-north.com/
http://planckpottery.com



__________________________________
Start your day with Yahoo! - Make it your home page!
http://www.yahoo.com/r/hs

Tony Ferguson on sat 29 oct 05


Gary,
Are you desiring flashing on the underside of the work? I wash my shelves with 90/10 alumina hydrate and epk and do a 50/50 like you for wadding (I think). I have not noticed any difference whether I have used sawdust, etc. with flashing on the bottom--for me it has been the claybody that cauzing more or less flashing underneath--as well as placement in the kiln too. Please do tell how things turn out. Good luck and skill.

Tony Ferguson


Gary Georger wrote:
For an anagana/cofffin woodfire we've been using a
50/50 or so mix of EPK and alumina hydrate ..but am
interseted in not so white/bald wading marks so I'm
going to experiment with adding sawdust,coffee,rice,
oats sand,grog ....anyone have recipe or guidelines
for wading and proportions?
much appriecated
Gary

http://www.washingtonpotters.org
http://www.gallery-north.com/
http://planckpottery.com



__________________________________
Start your day with Yahoo! - Make it your home page!
http://www.yahoo.com/r/hs

______________________________________________________________________________
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.


Tony Ferguson
...where the sky meets the lake...
Duluth, Minnesota
Artist, Educator, Web Meister
fergyart@yahoo.com
fergy@cpinternet.com
(218) 727-6339
http://www.aquariusartgallery.com
http://www.tonyferguson.net

---------------------------------
Yahoo! FareChase - Search multiple travel sites in one click.

Paul Herman on sat 29 oct 05


Gary,

We use this:

by weight,

1 fireclay

1 kaolin

1 sand or grog

sawdust to taste

Best,

Paul Herman

Great Basin Pottery
Doyle, California US
http://greatbasinpottery.com


On Oct 29, 2005, at 9:36 AM, Gary Georger wrote:

> For an anagana/cofffin woodfire we've been using a
> 50/50 or so mix of EPK and alumina hydrate ..but am
> interseted in not so white/bald wading marks so I'm
> going to experiment with adding sawdust,coffee,rice,
> oats sand,grog ....anyone have recipe or guidelines
> for wading and proportions?
> much appriecated
> Gary
>

John Britt on sat 29 oct 05


Gary,
Here are some recipes:


BRESNAHAN WADDING

AP Green Fireclay 50.00
Alumina Hydrate 20.00
Sand 30.00



Oat Bran Wadding

EPK -7 scoops
Fire Clay -7 scoops
Oat bran -7 scoops



Alumina Wadding

Epk -7 scoops
Silica -7 scoops
Alumina Hydrate -7 scoops


Not sure about this last one:


Wood wadding

SAND - 1 part
FIRE CLAY -1 part
SAWDUST -1 part
LIZELLA(or Yellow Ochre) - to taste



Best of luck!

John Britt
ww.johnbrittpottery.com

Lee Love on sun 30 oct 05


Tony F,

I might be mistaken, but I think Gary is talking about the white
marks left on the clay by the wads.

I polish them off with a whetstone. Tony, I remember you
mentioning trouble with smoothing porcelain. This traditional
whetstone grinding method might be safer on the bottom of porcelain.
You move the stone on the footring in a circular motion, first the flat
bottom, then the outside edge and lastly, the inside edge.

Another way is to avoid white marks is to use sea shells. The
white ones with lines on the exterior of the shell are best, especially
in earthquake country. ( during an earthquake a couple earthquakes ago
during a firing, I had a pot slip off of the smooth shells, while
every pot on the grooved shells stayed in place.) The shells
dissolve of when the bottom of the pot is placed in a bucket of
water. Don't play with the mush the shells turn into, because it is
somewhat caustic.
--
Lee Love
in Mashiko, Japan http://mashiko.org
http://seisokuro.blogspot.com/ My Photo Logs

"Where the spirit does not work with the hand, there is no art."