Hello Kate,

I have tried many years ago the recipy that follows , which I learned in =
one
workshop on glazes.
The result is translucent , but not quite charming in my reducting firi=
ng.
Maybe it will work better under oxidation.
Since you are experimenting, give it a try!

BRISTOL GLAZE ^6

Feldspar Potash 68,0
Calcium Carbonate. 10,0
Zinc Oxide 7,0
Kaolin 8,0
S=EDlica 7,0

Best regards to all, from Brazil.

Heloisa