Here is a recipe for an Opal Blue Glaze cone 9-10

Custer Feldspar 58.62
Whiting 23.44
EPK 15.41
Zircopax 2.51
100.0

Notes: Nice soft satin blue, copper flashes nicely


---------------------------------