Victoria,

There are many Flambe recipes listed in my book, but here is one:

JEFF'S RED Cone 9/10

Custer Feldspar 41.90
Whiting 8.40
Silica 26.20
Gerstley Borate 8.70
Barium Carbonate 4.40
Zinc Oxide 1.70
Dolomite 8.70

Tin Oxide 2.60
Copper Carbonate 0.50