search  current discussion  categories  glazes - specific colors 

noxema blue glaze

updated mon 26 jan 04

 

SCOTT YEIP on sat 24 jan 04


Went to the archives and found this.=20

NOXEMA BLUE Cone 4-6=20

Custer Feldspar 38.1=20
Dolomite 10.0=20
EPK 9.6=20
Silica 9.5=20
Gerstley Borate 9.5=20
Zinc Oxide 9.4=20
Cobalt Carb 3.5=20

It is not the same as yours as it has less siica and it doesn't add up =
either! It's the only blue glaze that I can find under that description =
in the archives.