Get ISBN : 0-967-562-0-9

Kohler slip

12 FC kaolin
16 C& C Ball Clay
25 L-1 Ball Clay
5 Black Charm Ball Clay
2 Bancy Black Ball Clay
18 NC-4 Feldspar
22 Flint


40 % Water
0.25 - 0.5 %Sodium silicate