I thought to myself: "Could I send a recipe with 38% raw ball clay? Is
it me?"
I rebuilt the recipe properly.
A historical preview: When I played with Marty Anderson's butterscotch
there was not spodumen in Israel.
Now I could buy it so I added it to the more stable source of lithium
carbonate.



The revised recipe(A decorative glaze)
DRY YELLOW PUMPKIN
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Ferro 3134 18.00
Dolomite 19.00
kaolin CC31 24.00
kaolin CC31 calcined 16.00
spodumen 16.00
Quartz 8.00
Rutile 6.00
Titanium Dioxide 14.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.127 2.90%
CaO 0.507 9.15%
MgO 0.247 3.20%
Li2O 0.119 1.14%
Al2O3 0.552 18.10%
B2O3 0.171 3.84%
SiO2 2.237 43.24%
TiO2 0.717 18.42%
K2O 0.036 1.09%
Na2O 0.091 1.81%
Al:Si 4.05
Expan. 8.06
ST 396.36
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,


Now I will try to adjust is for our American fellows as the CC31 has
more flux and less alumina than the EPK
The next recipe was not tested (A decorative glaze too!)

DRY YELLOW PUMPKIN
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Ferro 3134 16.60
Dolomite 18.00
EPK 22.70
Alumina Hydrate 8.30
spodumen 15.60
Flint 13.70
frit 3110 5.10
Rutile 6.00
Titanium Dioxide 14.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.127 2.54%
CaO 0.512 9.15%
MgO 0.241 3.10%
Li2O 0.120 1.14%
Al2O3 0.556 18.02%
B2O3 0.170 3.77%
SiO2 2.263 43.31%
TiO2 0.745 18.97%
K2O 0.004 0.13%
Na2O 0.122 2.41%
Al:Si 4.07
Expan. 8.09
ST 396.24
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
http://members4.clubphoto.com/ababi306910/981929 The last slide
Yours forever

Ababi Sharon

Glaze addict

Kibbutz Shoval Israel

ababisha@shoval.org.il

http://members4.clubphoto.com/ababi306910

http://www.matrix2000.co.nz/Matrix%20Demo/Ababi.htm