Ababi on wed 12 mar 03


Ababi's ASH AND SOIL#17B ^6 oxidation decorative glaze
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

soil 22.50
pine ash 22.50
Laguna Borate 11.30
RedArt Clay 14.50
Quartz 19.30
EPK Kaolin 10.00
Tin Oxide 5.00
Red Iron Oxide 1.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.374 10.83%
CaO 0.445 8.88%
MgO 0.181 2.59%
Al2O3 0.277 10.03%
P2O5 0.041 2.06%
B2O3 0.127 3.15%
SiO2 2.903 62.07%
TiO2 0.013 0.38%
K2O 0.225 7.54%
Na2O 0.149 3.29%
Al:Si 10.50
About 4% iron
Expan. 8.11
ST 332.93
This was glaze 17 in the grid. I made it wrong, the red clay equivalent to redart has too
low alumina. Because of this reason, I did it in Curries site than changed the kaolin to
the red clay.
Sieve and wash the ash twice. Sieve the soil in 30- 80 mesh screen. add CMC apply
thin and thick.
Was tested only ones!