search  current discussion  categories  glazes - cone 8-10 

cone 10 reduction glaze

updated wed 22 jan 03

 

Eve Juliano on mon 20 jan 03


I seem to have lost my glaze receipe for V.C. cobalt blue glaze at cone
10 reduction. Doe sanyone have that receipe that I believe I obtained
from this list about 8 years ago.

Thanks ----Eve Juliano

John Weber on tue 21 jan 03


I don't know if this is the glaze you are looking for but this is from the
GlazeBase list. Looks like the Silica is too low:
V.C. AA COBALT BLUE
Cornwall Stone 46
Whiting 34
EPK 20
---------------
Cobalt Carbonate 2
===============================
Na2O 0.06 Al2O3 0.35 SiO2 1.71
K2O 0.05 P2O5 0.00
MgO 0.00 TiO2 0.00
CaO 0.84 Fe2O3 0.00
CoO 0.04

Alumina:Silica ratio is 1.00:4.87
Neutral:Acid ratio is 1.00:4.90
Alk:Neut:Acid ratio is 1.00:0.35:1.72

Expansion: 82.9 x 10e-7 per degree C