Joyce and others who use VC's Handbook,
At a weekend workshop Val Cushing corrected a glaze recipe on page 138 of the 3rd edition of his handbook. His correction is this:
VC Good Color Satin Matt ^9-10
Nepheline Syenite 27
Lithium Carbonate 5
Gerstley borate 18
Wollastonite 8
Talc 14
EPK 20
Flint 8

Saundra in Zirconia, NC