Ababi on sat 28 sep 02


Hello Clayart!
The last glaze in my article, as I read it from the fax I have got:
Kaolin 30.5
Strontium carbonate 15.7
Wollastonite 18.1
cryolite 10.5
tin oxide 5
copper oxide 3

The silica was lost on the clipboard.
I tested this glaze. The numbers bellow were brought to 100% + tin and copper.

The new names tells all!
STRONTIUM4B TURQU
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

ENGLISH KAOLIN CC31 40.80
STRONTIUM CARBONATE 21.00
Wollastonite 24.20
Cryolite 14.00
Tin Oxide 6.70
copper oxide 4.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.256 8.97%
CaO 0.406 12.19%
MgO 0.020 0.43%
SrO 0.318 17.63%
Al2O3 0.410 22.33%
SiO2 1.196 38.46%
K2O 0.027 1.37%
Na2O 0.229 7.60%
Al:Si 2.92
Expan. 10.52
ST 402.55
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

On white stoneware sprayed, turquoise matte coat
delicate.

Now to the real and correct recipe

STRONTIUM4B TURQUOISE
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

SILICA 25.20
ENGLISH KAOLIN CC31 30.50
STRONTIUM CARBONATE 15.70
Wollastonite 18.10
Cryolite 10.50
Tin Oxide 5.00
copper oxide 3.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.257 6.41%
CaO 0.406 8.68%
MgO 0.020 0.31%
SrO 0.318 12.55%
Al2O3 0.409 15.92%
SiO2 2.448 56.13%
K2O 0.027 0.98%
Na2O 0.229 5.43%
Al:Si 5.98
Expan. 8.53
ST 381.09

Silky shine when sprayed on white stoneware.
this glaze will slowly will take the place of Behrens's stony matte as I will learn to use
it correctly.

You can try it with 3 RIO instead of the copper. I will do it within two weeks

Ababi Sharon
Glaze addict
Kibbutz Shoval Israel