silver glaze hope it works!

updated fri 9 aug 02

 

Ababi on thu 8 aug 02


http://members4.clubphoto.com/_cgi-bin/getImage.pl?imgID=11832070-06af&trans=
Do not forget the "equal"
On porcelain: clear silvery motteled sometimes baige.
The silvery look thanks to unsieved glaze and EZE spraygun.
Out of a test in Lana Wison's book I have learnt that one spoon ruitle 7 grams
and one spoon bone ash 24 gram are
giving
strong matte orange.
I made sevaral tests, adding this combinations to different bases. Never succeeded
but got sometimes nice glazes.

I refomulated it I hope it will work for you

SILVER GLAZE HOPE IT WORKS!
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

SILICA 21.70
Bone Ash 21.70
ENGLISH KAOLIN CC31 7.60 (Any kaolin)
ZINC OXIDE 9.20
rutile 7.60
Custer feldspar 32.10
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.139 4.49%
CaO 0.561 12.03%
MgO 0.001 0.02%
ZnO 0.300 9.33%
Al2O3 0.215 8.37%
P2O5 0.185 10.07%
SiO2 2.100 48.27%
TiO2 0.243 7.42%
K2O 0.097 3.50%
Na2O 0.041 0.98%
Al:Si 9.78
Expan. 7.46
ST 339.39
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,