June Perry on thu 16 may 02


This may be the one you're looking for.

#167 SHANER YELLOW RED 9-10 REDUCTION YELLOW WITH RED SPECKS MATT. * I
believe it also works in salt firings.

ZIRCOPAX 23
POTASH FELDSPAR 49
WHITING 20
TALC 4
BONE ASH 4

ADD:
IRON OXIDE 4%,
BEN A GEL 1/4%