search  current discussion  categories  glazes - misc 

my favorite glaze

updated wed 8 may 02

 

Ababi on tue 7 may 02


Out of 200 most popular:

STONYEARTH GREEN-BEHRENS: A DECORATIVE GLAZE
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1201 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Bone Ash 8.40
Nepheline Syenite 18.70
Magnesium Carb Light 2.00
Wollastonite 8.90
Earth 11.80
STRONTIUM CARBONATE 32.50
ENGLISH KAOLIN CC31 15.30
SILICA 2.50
Tin Oxide 5.60
COPPER OXIDE 3.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.112 4.51%
CaO 0.340 10.64%
MgO 0.078 1.75%
SrO 0.470 27.15%
Al2O3 0.241 13.72%
P2O5 0.058 4.58%
SiO2 1.119 37.50%
TiO2 0.003 0.14%
K2O 0.036 1.89%
Na2O 0.076 2.62%
Al:Si 4.63
Expan. 9.06
ST 404.12
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Clay Body Dark , apply partly to show the difference
Colour "Dirty" turquoise
Glaze Type matte dry
Opacity yes
Texture un smooth
Stability I would not test it for vinegar
Fit lovely
Last changed: Today , Nephalin instead of my local Italian feldspar
Status Static
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,
Comment: I use Loess soil. might get different result out of yours.
See it in one of my glaze test pages ( and win a bottle of coca cola)
Ababi Sharon
Kibbutz Shoval- Israel
Glaze addict
ababisha@shoval.org.il
http://members4.clubphoto.com/ababi306910/