Ababi on fri 19 apr 02


When I tried last year to make cups, I thought I should use inside a
harmless glaze, without knowing it should be called liner.
How this glaze looks to you?
From Stephen's pottery web site
http://members.bellatlantic.net/~spilacho/

^6 OX CLEAR OF DALE HUFFMAN
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1222 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Nepheline Syenite 40.00
GB Average 10.00
SILICA 30.00
Calcium Carbonate 10.00
EPK Kaolin 7.00
Bentonite 1.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.374 7.41%
CaO 0.584 9.38%
MgO 0.043 0.49%
Al2O3 0.425 12.41%
B2O3 0.172 3.42%
SiO2 3.884 66.88%
K2O 0.084 2.27%
Na2O 0.290 5.15%
Al:Si 9.14
Expan. 7.56
ST 344.92
Comment: I might have to spry it, when I made it was too thick, on the
border of not nice.
As clear and with tin or ultrox
Thank you very much for patient (if you reached to this part of the
letter)
Ababi Sharon
Kibbutz Shoval- Israel