search  current discussion  categories  glazes - misc 

cone 03 clear glaze +^2+^3

updated sun 17 mar 02

 

Ababi on sat 16 mar 02


Hello Liz Here are two Recipes of mine ^6 glazes that through a special
function in Matrix I found they can fire in 1010C
Might be kower you must try. use them as they are or desmist the
tiatnium, nickele Red iron oxide tin and ultrox

MY GREEN GLAZE
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1201 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cryolite 20.00
SILICA 30.00
FRIT 3195 20.00
ZINC OXIDE 15.00
ENGLISH KAOLIN CC31 15.00
Nickel Oxide 2.00
Titanium Dioxide 5.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.401 10.72%
CaO 0.098 2.34%
MgO 0.002 0.03%
ZnO 0.436 15.10%
Al2O3 0.299 12.95%
B2O3 0.155 4.60%
SiO2 1.839 47.05%
TiO2 0.149 5.05%
K2O 0.011 0.42%
Na2O 0.390 10.30%
NiO 0.0633 2.01%
Al:Si 6.16
Expan. 9.65
ST 341.94
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

And:
FALLS CREEK SHINO ABABI.#6
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Cone 6 1201 deg.C. -
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

FRIT 3134 40.00
RED CLAY (GRT) 30.00
Dolomite 5.00
ULTROX 10.00
Tin Oxide 5.00
Red Iron Oxide 1.00
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Seger Weight%
KNO 0.287 7.20%
CaO 0.606 12.54%
MgO 0.107 1.59%
Al2O3 0.194 7.30%
B2O3 0.463 11.89%
SiO2 2.291 50.83%
ZrO2 0.190 8.64%
K2O 0.052 1.82%
Na2O 0.235 5.37%
Al:Si 11.81
Expan. 7.57
ST 323.02
,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,,

Of course they look better in ^6
So here are two glazes for ^2 and ^3
---------- Original Message ----------

>Hi Liz,
>I teach at Foothill H.S. in Pleasanton but live in Walnut Creek and do
>my shopping at Leslie's Ceramics in Berekely,Ca. on San Pablo ave.They
>have a good c/o6 clear that I use over underglaze as well as adding
>Cobalt carb, copper carb and both with blk. iron ox for a darker
>version. Pretty versitile. I double the cost of the clay to the
students
>to cover glaze, tools,etc. It works. Mike Gordon

>_______________________________________________________________________
_
>______
>Send postings to clayart@lsv.ceramics.org

>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/

>Moderator of the list is Mel Jacobson who may be reached at
>melpots@pclink.com.