Cindy Strnad on sun 3 mar 02


I'll post some glaze tests. Here is how they were fired:

150=BAF/hr to 2100
50=BA/hr to 2160 (cone 6 half-way down)
Hold for 15 minutes
Cool naturally to 1900=BA
Cool at 100=BA/hr to 1500=BA
Cool naturally to room temperature (12=BA below zero in this particular
case--brrrr! Actually, I only let the pots get down to 60=BA. They felt n=
ice and
warm.)

I fired so slowly because I had a large piece with a minor glaze flaw to =
re-fire
and I didn't want it to blow up. Normally I would have fired at 200=BAF/h=
r in the
first phase, which is also pretty slow, but that's how I'm doing it at th=
e
moment.

All pieces were brown stoneware clay with grog.
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
Cindy Strnad
Earthen Vessels Pottery
RR 1, Box 51
Custer, SD 57730
USA
cindy@earthen-vessels-pottery.com
http://www.earthen-vessels-pottery.com
CM Critique discussion forum
http://www.earthen-vessels-pottery.com/toforum.html