> does any one know a recipe for
> a fake flashing avery slip that looks good in a wood fireing?

Andy -
This is one I got from Cheri Glaser.

Fake Avery
Neph Sye 20
Grolleg 30
Calcined EPK 30
EPK 20
Bent. 2

It is specifically intended for application to bisque-fired wares to be
fired in salt and wood firing, and we have had good luck with it.
Best wishes -
- Vince

Vince Pitelka
Appalachian Center for Crafts
Tennessee Technological University
1560 Craft Center Drive, Smithville TN 37166
Home - vpitelka@dtccom.net
615/597-5376
Work - wpitelka@tntech.edu
615/597-6801 ext. 111, fax 615/597-6803
http://www.craftcenter.tntech.edu/

rohde on sat 10 nov 01


does any one know a recipe for=20
a fake flashing avery slip that looks good in a wood fireing?

thanks andy

Ruth Ballou on sat 10 nov 01


50 EPK / 50 OM 4 Ball Clay





>does any one know a recipe for
>a fake flashing avery slip that looks good in a wood fireing?

Lana Reeves on sat 10 nov 01


does any one know a recipe for
a fake flashing avery slip that looks good in a wood fireing?

Try Tile 6 clay with a little iron [Redart, Newman Red]


____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.