Here's one from my glaze page which is manganese free and should work in
reduction:

Glaze name: H38-40 (black gloss)

Cone: 8 - 10
Firing: Ox. or Red.
Recipe:

Potash feldspar 38.92
Silica 28.02
Kaolin 10.06
Dolomite 4.55
Bone ash 4.55
Whiting 13.91
-------- --------
Totals: 100.00 100.00

Also add:

Red iron oxide 4.55
Cobalt carbonate 1.00
Copper carbonate 0.55

--