Jeff Zamek's
Black Friday Glaze Cone 6

Nepheline Syenite 270x 20
Whiting 15
EPK 18
Ferro frit #3124 20
Flint 325x 17
Bone ash (animal ash) 10
Mason black stain #6600 12