search  current discussion  categories  glazes - misc 

fw: misplaced recipe - gremlins strike again?

updated wed 5 sep 01

 

Wade Blocker on tue 4 sep 01


----------
> From:
> To: Ceramic Arts Discussion List
> Subject: Re: Misplaced recipe - Gremlins strike again?
> Date: Tuesday, September 04, 2001 3:05 PM
>
> Lori,
> This is Chappell's glaze 2nd one from the top on the left
>
>
> CRG-6 artificial Copper red cone 2
>
> Felspar, Kona F4 34.0
> Borax 29.2
> Fluorspar 6.6
> Kaolin (florida) 12.4
> Silica 17.8
> Tin oxide 2.0
> Cu carb 0.5
> Silicon carbide 200 mesh 0.5
> Bentonite l.0
> CMC one tsp
>
>
>
>
> Mia