sun valley glaze

updated thu 23 aug 01

 

Hannah on wed 22 aug 01


To Imzadi and others interested in the Sun Valley recipe:


SUN VALLEY CONE 10 REDUCTION

Custer Feldspar....................29.6 =20
Flint .....................................23.3 =
=20
Whiting.................................18.9 =
=20
Talc......................................10.3
EPK......................................l5.3
Rutile......................................7.6


I've enjoyed this glaze. It will look different on light or dark clay =
but usually is interesting. It becomes a richer blue over orange =
glazes or combined with other rutile glazes. Less blue and more cream =
on light clay.

Good luck with it-
Hannah