Some I have sent here as a collection

Emily's Purple
================
Custer feldspar..... 36.56 32.27%
Gerstley borate..... 19.35 17.08%
OM#4 Ball clay...... 11.83 10.44%
Talc................ 15.05 13.29%
Flint............... 10.75 9.49%
Dolomite............ 6.45 5.69%
ULTROX.............. 10.00 8.83%
cobalt o........... 3.30 2.91%
========
113.30

CaO 0.31* 6.66%
MgO 0.49* 7.45%
K2O 0.11* 3.81%
Na2O 0.09* 2.14%
TiO2 0.00 0.01%
ZrO2 0.14 6.53%
Al2O3 0.27 10.55%
B2O3 0.22 5.67%
SiO2 2.50 56.96%
Fe2O3 0.00 0.23%

Si:Al 9.17
SiB:Al 9.95
Expan 6.26

Emily's Purple 2
================
BALL CLAY (AK)...... 23.80 21.01%
TALC................ 13.88 12.25%
DOLOMITE............ 11.02 9.73%
LAGUNA BORATE....... 6.53 5.77%
FRIT F4(Colorobia).. 26.11 23.05%
WHITING............. 0.91 0.81%
QUARTZ.............. 17.73 15.65%
ULTROX.............. 10.00 8.83%
cobalt o 3.3........ 3.30 2.91%
========
113.30

CaO 0.32* 6.90%
MgO 0.49* 7.65%
K2O 0.07* 2.49%
Na2O 0.13* 3.14%
TiO2 0.00 0.03%
ZrO2 0.13 6.40%
Al2O3 0.27 10.75%
B2O3 0.22 6.04%
SiO2 2.40 56.34%
Fe2O3 0.00 0.24%

Text1 10.60
Si:Al 8.90
SiB:Al 9.72
Expan 6.26

Notes:
Excellent glaze!


I did not shive it just with a fast drill and jiffy mixer
frit F4 colorbia
might be available over your under "Hobby -Colorobbia"
similar somehow to 3124:




FRIT F4(Colorobia).. 100.00 100.00%
========
100.00

CaO 0.11 6.01%
K2O 0.10 8.98%
Na2O 0.18 11.00%
Al2O3 0.09 8.99%
B2O3 0.22 15.00%
SiO2 0.83 50.01%

Si:Al 9.44
SiB:Al 11.88
Expan 10.90

There is a version of this glaze with tin:
From the Ceramic web, probably the original, with 5 tin, I don't remember if
the silica is different.
But I am an ultrox addict!

PURPLE^6
========
NEPHELINE SYENITE... 41.40 40.59%
DOLOMITE............ 11.70 11.47%
MAGNESIUM CARBONATE. 5.40 5.29%
WHITING............. 4.50 4.41%
QUARTZ.............. 27.00 26.47%
GERSTLEY BORATE..... 10.00 9.80%
*COBALT CARBONATE.... 2.00 1.96%
========
102.00

CaO 0.39* 8.43%w 10.69%m
MgO 0.34* 5.25%w 9.26%m
K2O 0.06* 2.00%w 1.51%m
Na2O 0.21* 4.97%w 5.70%m
SrO 0.00* 0.01%w 0.01%m
Al2O3 0.25 9.92%w 6.92%m
B2O3 0.11 2.92%w 2.99%m
SiO2 2.32 53.19%w 62.90%m
Fe2O3 0.00 0.06%w 0.03%m

Text1 8.64
L.O.I. 13.23
Si:Al 9.10
SiB:Al 9.53
Expan 7.56
You can of coarse change the amount of the cobalt!
Notes:
FROM ^10

from a recipe of Ruth Ballou rballou@bellatlantic.net


The first time I made the original recipe, it tuned out in ^6 not mature,
beautiful light purple,pastel- like appearance.
You may find it in the archives.
Emily, can be a nice white, but ONLY white the magnesia kills all oxides
except cobalt!

I found out that if I use the "West & Gerrow" expansion of matrix give me
similar results to the expansion of Insight (for an easier comparing between
these two great programs!

Ababi