I forgot to post this glaze. This is the glaze I applied over top of
Edwards 4.3.2.1 Matte OM-4 base that I added the colorants for the yellow.

Chris Wolff's Cream Gloss cone 6

45.0 Frit 3134 F12
5.0 Talc
19.0 Custer Feldspar (used G-200)
6.0 Cornwall Stone
14.5 EPK (Kaolin)
10.5 Flint (Silica)

Opaque cream under very shiny clear

Marianne Lombardo
Omemee, Ontario, Canada