search  current discussion  categories  glazes - specific colors 

oxy weathered bronze green

updated thu 7 jun 01

 

Jim and Marge Wade on tue 5 jun 01


Here's the recipe. It's from Pete Pinnell.

Weathered Bronze Green ^6 Ox

Lithium Carb 1
Stronium Carb 20
Neph Sye 60
Ball Clay 10
Flint 9
Titanium Oxide 5
Copper Carb 5



> From: Jim Innes
> Reply-To: Ceramic Arts Discussion List
> Date: Wed, 6 Jun 2001 08:27:55 +1200
> To: CLAYART@LSV.CERAMICS.ORG
> Subject: Oxy weathered bronze green
>
> I have been unable to find the formula for this often discussed glaze in the
> archives. Could someone please give me the formula. Many thanks. Jim
>
> ______________________________________________________________________________
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.

Marianne Lombardo on tue 5 jun 01


I am pretty sure that glaze is on www.frogpondpottery.com if memory serves
me correctly.

Marianne Lombardo
Omemee, Ontario, Canada
email: mlombardo@nexicom.net

>Subject: Oxy weathered bronze green
>I have been unable to find the formula for this often discussed glaze in
the archives. Could someone please give me
>the formula. Many thanks. Jim

Jim Innes on wed 6 jun 01


I have been unable to find the formula for this often discussed glaze in =
the archives. Could someone please give me the formula. Many thanks. Jim