search  current discussion  categories  materials - clay 

tr: pour ababi...(from gien earthenware factory)

updated wed 23 may 01

 

Edouard Bastarache on mon 21 may 01


Hello Ababi,

for your info from the famous Gien factory.


Later,

Edouard Bastarache
Irr=E9ductible Qu=E9becois
Sorel-Tracy
Dans / In "La Belle Province"
edouardb@sorel-tracy.qc.ca
http://www.sorel-tracy.qc.ca/~edouardb/
----- Message d'origine -----
De : Denis Caraty
=C0 : Edouard Bastarache
Envoy=E9 : 21 mai, 2001 09:55
Objet : Pour Ababi...


>
> Salut Ed,
>
> Voici la fiche technique correspondant au Kaolin D'Arvor (kaolinor 1C)s=
ur
le
> site de la soci=E9t=E9 DAM min=E9raux :
> http://www.dam-mineraux.fr/fiches_tech/Arvor/KAOLINOR_1C.htm
> Autres kaolins :
> http://www.dam-mineraux.fr/fiches_tech/acceuil_mineraux/sub/email.htm
> Pr=E9sentation :
> http://www.dam-mineraux.fr/fiches_tech/acceuil_mineraux/sub/Kaolin.htm
>
> Contact :
> http://www.dam-mineraux.fr/uk/Contacts.htm
>
> Appeler pour cette affaire :
>
> Camille Le Cheviller
> Responsable Commercial Export
> Kaolins d=92Arvor Kergantic
> 56276 PLOEMEUR
> T=E9l. : +33 (0) 2 97 86 16 16
> Fax : +33 (0) 2 86 16 11
> e-mail : mailto:kaolins.arvor@adresse.fr
>
>
>
> Bonne transmission, a bientot.
>
> Denis Caraty
> Soci=E9t=E9 : Fa=EFenceries de Gien
> 78, place de la victoire, 45500 Gien, FRANCE
> Fax : (33) 2 38 67 92 36
> mailto:dcaraty@gien.com
> http://www.gien.com
>
>

Ababi on tue 22 may 01


Hello Eddourd!
Thank you very much!
Do you know if this is a plastic kaoilin?
Here is the copied page:
Ababi dans le Negev nordique où les oiseaux sont des singings que les vaches
donnent le lait et et aidez ou des jardins aussi! Remerciez Dieu, rapport
très bon
vec nos voisins de bédouin.

(.....Ababi in the Northern Negev where birds are singings cows are giving
milk and and help our gardens too! Thank God, pretty good
relationship with our Bedouin neighbors.)




Les produits GMH


KAOLINOR 1C

ANALYSE CHIMIQUE
CHEMICAL ANALYSIS (%)


SiO2
47.4

Al2O3
36.6

Fe2O3
0.8

TiO2
0.1

Na2O
0.1

K2O
1.2

CaO
0.02

MgO
0.2
pF 12.5


PROPRIETES PHYSIQUES
PHYSICAL PROPERTIES

HUMIDITE < 14 %
(Humidity)

DENSITE REELLE 2,6
(Specific gravity)

INDICE DE REFRACTION 1,55
(Refractive index)

SURFACE SPECIFIQUE BET 13 m²/ g
(Specific surface area) RETRAIT TOTAL A 1200°C 5.2 %
(Shrinkage at 1200°C)

ABSORPTION D'EAU 8 %
(Water absorption)

BLANCHEUR APRES CUISSON A 1200°C
BRIGHTNESS AFTER FIRING AT 1200°C

Filtre bleu R457 nm 88
(Blue filter R457 nm)

ANALYSE GRANULOMETRIQUE
PARTICLE SIZE DISTRIBUTION

> 63 µm < 500 ppm
< 20 µm 100 %
< 10 µm 95 %
< 5 µm 81 %
< 2 µm 59 %

RESISTANCE MECANIQUE
BENDING STRENGTH

Après séchage à 100°C 8Kgf/cm²
(After drying at 100°C)


The technical details contained in this data sheet are given in all good
faith for indicative purposes only, and do not constitute a guarantee by
DAM. The Central Laboratory of the DAM Group will supply any additional
information required. Characteristics shown in Italics correspond to those
which are routinely controlled against specification. The remaining
characteristics are indications of the inherent properties of the exploited
minerals.




Siège Social et Usine : Kergantic - 56276 PLOEMEUR Cedex- France
Tél. +33 (0) 2 97 86 16 16- Fax + 33 (0) 2 97 85 23 34
http://www.dam-mineraux.fr contact@dam-mineraux.fr




Ababi Sharon
ababisha@shoval.ardom.co.il
http://members4.clubphoto.com/ababi306910/
http://www.milkywayceramics.com/cgallery/asharon.htm
----- Original Message -----
From: "Edouard Bastarache"
To:
Sent: Monday, May 21, 2001 5:40 PM
Subject: Tr: Pour Ababi...(From Gien earthenware factory)


Hello Ababi,

for your info from the famous Gien factory.


Later,

Edouard Bastarache
Irréductible Québecois
Sorel-Tracy
Dans / In "La Belle Province"
edouardb@sorel-tracy.qc.ca
http://www.sorel-tracy.qc.ca/~edouardb/
----- Message d'origine -----
De : Denis Caraty
À : Edouard Bastarache
Envoyé : 21 mai, 2001 09:55
Objet : Pour Ababi...


>
> Salut Ed,
>
> Voici la fiche technique correspondant au Kaolin D'Arvor (kaolinor 1C)sur
le
> site de la société DAM minéraux :
> http://www.dam-mineraux.fr/fiches_tech/Arvor/KAOLINOR_1C.htm
> Autres kaolins :
> http://www.dam-mineraux.fr/fiches_tech/acceuil_mineraux/sub/email.htm
> Présentation :
> http://www.dam-mineraux.fr/fiches_tech/acceuil_mineraux/sub/Kaolin.htm
>
> Contact :
> http://www.dam-mineraux.fr/uk/Contacts.htm
>
> Appeler pour cette affaire :
>
> Camille Le Cheviller
> Responsable Commercial Export
> Kaolins d'Arvor Kergantic
> 56276 PLOEMEUR
> Tél. : +33 (0) 2 97 86 16 16
> Fax : +33 (0) 2 86 16 11
> e-mail : mailto:kaolins.arvor@adresse.fr
>
>
>
> Bonne transmission, a bientot.
>
> Denis Caraty
> Société : Faïenceries de Gien
> 78, place de la victoire, 45500 Gien, FRANCE
> Fax : (33) 2 38 67 92 36
> mailto:dcaraty@gien.com
> http://www.gien.com
>
>

____________________________________________________________________________
__
Send postings to clayart@lsv.ceramics.org

You may look at the archives for the list or change your subscription
settings from http://www.ceramics.org/clayart/

Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.