search  current discussion  categories  glazes - cone 4-7 

glaze test for candle satin matt, c6, oxidation

updated fri 22 dec 00


Alisa and Claus Clausen on thu 21 dec 00

Candle Satin Matt C6, oxidation
Source: Clayart
Comments: Alumina matt, gets shiner with added oxides.

Tested on mid range, iron flecked stoneware, fired to 1220c, oxidation.

42 G200
19 Talc
9 Dolomite
15 EPK
6 Silica

Subbed local spar for G200.

Resulted in clear gloss with pool of white and blue opal in center in of =
test bowl. Cobalt and Iron oxide
washes underneath showed from underneath glaze as they were painted.

Best regards,
Alisa in Denmark