glaze test for c6 ron roy revision ez clear with frit 169

updated fri 22 dec 00

 

Alisa and Claus Clausen on thu 21 dec 00


EZ clear with Frit 169
=20
Tested on mid range, iron flecked stoneware, fired to 1220c, oxidation.
=20
Original Receipe
48 BB
22 EPK
30 Silica
=20
Tested Receipe
34 Frit 169
12Wallastonite
24 EPK
30 Silica
=20
Resulted in gloss clear, stable glaze. Underlying cobalt and iron wash =
remained stable under glaze.
=20
Best regards,
Alisa in Denmark