Tested on white mid range stoneware, fired to 1220c, oxidation.

56.7 Alberta Slip
18.69 Gerstely Borate
9.35 Silica
6.54 Lithium Carb.
9.35 Superpax
4.67 Tin Oxide

Receipe used
57 Oldenwalder clay
19 Local Frit
9 Silica
7 Lithium Carb.
9 Zircopax
5 Tin ox.

Resulted in a stable, gloss, medium brown.