search  current discussion  categories  glazes - cone 4-7 

glaze test for charcola satin matt cone 6, oxidation.

updated tue 28 nov 00

 

Alisa and Claus Clausen on sun 26 nov 00


Source:
Ceramics Monthly September 2000 (John Hesselberth and Ron Roy)
derived from Tony Hansen's Matt Base.

Receipe
23.2 Wollastonite
31.0 Frit 3124
31.7 EPK
14.0 Flint

ADD
6 Rutile
10. Mason Stain 1.0

Substitutions
All measurements rounded off at the next highest decimal.
Local frit for Frit 3124
Used universal stain powders, medium grey.

Resulted in stable, matt grey with a bluish hue. =20

Personal:
Very attractive glaze with a good feel. Will try with other stain =
colors.

Best regards,
Alisa in Denmark