search  current discussion  categories  wanted/for sale - wanted 

looking for cone 5&6 glazes

updated sun 19 nov 00

 

Monica Long on fri 17 nov 00


I am just starting out as a potter and I am trying to build up my glaze
recipe book. I have an order for a purple matte bowl set and I can't find
any recipes, or evem prepared purple matte glazes. I would also love a
pewter, or mettalic slate grey glaze, and any other nice cone 5 or 6 glazes.
Thankyou
_________________________________________________________________________
Get Your Private, Free E-mail from MSN Hotmail at http://www.hotmail.com.

Share information about yourself, create your own public profile at
http://profiles.msn.com.

Diane G. Echlin on fri 17 nov 00


Monica, go to this web page. oodles of recipes. Look for "pike's Oatmeal" and
there is a variation for purple.
Diane in CT

http://members.aol.com/goodrichdn/

Monica Long wrote:

> I am just starting out as a potter and I am trying to build up my glaze
> recipe book. I have an order for a purple matte bowl set and I can't find
> any recipes, or evem prepared purple matte glazes. I would also love a
> pewter, or mettalic slate grey glaze, and any other nice cone 5 or 6 glazes.
> Thankyou
> _________________________________________________________________________
> Get Your Private, Free E-mail from MSN Hotmail at http://www.hotmail.com.
>
> Share information about yourself, create your own public profile at
> http://profiles.msn.com.
>
> ______________________________________________________________________________
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.

Brenda Beeley on sat 18 nov 00


From: Monica Long
Subject: looking for cone 5&6 glazes

>I am just starting out as a potter and I am trying to build up my glaze
>recipe book. I have an order for a purple matte bowl set and I can't find
>any recipes, or evem prepared purple matte glazes. I would also love a
>pewter, or mettalic slate grey glaze, and any other nice cone 5 or 6 glazes.

Dear Monica,
These were posted previously on Clayart. I haven't tried them.
Good luck, Brenda

Oxidation.

Purple ^6
Custer spar 37
Gerstley Borate 12
Dolomite 6
Talc 14
EPK 5
Silica 23
Zinc Oxide 3
Cobalt Carb 3
Bentonite 2

a true purple at ^6, more blue at ^7 and ^8

Sea Blue ^6-7
Colemanite 15.65
Lithium 6.96
Potspar 42.61
EPK 13.04
Flint 21.74
Zinc 20.89
Nickle Ox 1.3

Oil Spot Green/Blue ^6
3134 50
EPK 40
Silica 20
Cobalt Carb 3
Rutile 5

LA Mot ^6 John Britt via Susan @ Ceramics Canada, Calgary
Custer 41.75
Wollastonite 17.48 (originally calls for Calcium Carb)
EPK 15.53
Zinc 6.8
Flint 18.45
Rutile 5.82

this is a warm yellow and a nice surface at ^6.....some pinholing with a
fast firing
Joy, this works nicely over ^6 Purple fired to ^8 or 9 (not so nice at ^6)