Marcia Selsor on fri 3 nov 00


Dear gayle,
I have no crazing on my porcelain with your recipe. I used Geo. kaolin
if that makes a difference. I think it's the clay body. I also tried
Malgrems faux celedon to ^6 eletric. It was much deeper (too deep for my
taste) but very nice texture.-could cut the copper for my taste.
Also tried that Mimuzo recipe in this month's CM. tried some stains. I
had an old bag of Crinson Mason stain. On Gayle's recipe it was red, on
Mimuzo it was textured mauve. The degussa colors on Gayle's came out
brilliant. -orange .
Marci
Recipes
Marci's clear
Whiting 10.5
Neph. Syn 25.8
EPK 18.8
Silica 31.1
Gerst. Bor. 4.6
add .75 copper carb for faux celedon in electric
add same with 1% tin for red in gas.
use 1.5 % Iron oxide for celedon in Gas

Gayle's Faux Celedon
F-4 50
Wollastonie 20
Kaolin 10
Silica 10
Gerst. Bor 10
Copper carb .5
Black stain .2

Malgrem and Mimuzo are in Oct and Nov CM and don't want to impinge on Copyright









--
Marcia Selsor