Here is Marty's Butterscotch^6 revised by RRoy.

RR Revision for Marty's Butterscotch FOODSAFE
=============================================
FRIT 3134........... 25.00 20.49%
DOLOMITE............ 12.00 9.84%
LITHIUM CARBONATE... 2.00 1.64%
G200 spar -......... 10.00 8.20%
BALL CLAY (AK)...... 26.00 21.31%
SILICA.............. 25.00 20.49%
Titanian Dioxide -.. 9.00 7.38%
Rutil -............. 4.00 3.28%
TITANIUM DIOXIDE... . 9.00 7.38%

========
122.00

CaO 0.40* 7.23%w 8.79%m
Li2O 0.07* 0.67%w 1.53%m
MgO 0.39* 5.10%w 8.64%m
K2O 0.03* 0.95%w 0.69%m
Na2O 0.12* 2.36%w 2.60%m
TiO2 0.41 10.55%w 9.01%m
ZrO2 0.00 0.03%w 0.02%m
Al2O3 0.26 8.62%w 5.76%m
B2O3 0.21 4.73%w 4.64%m
SiO2 2.62 51.29%w 58.21%m
Fe2O3 0.01 0.31%w 0.13%m

L.O.I. 8.17
Si:Al 10.10
SiB:Al 10.91
Expan 6.72

I tested the glaze, with my frit. There is a small different in the
formulas
The result was a gloss and a bit uneven color, kind of light yellow and pale
yellow spots, but a good and workable glaze.