Here's a blue, very simple, very blue:
It's so new in my testing I haven't named it!
40% custer feldsapr
30 silica
20 calcium carbonate (whiting)
10 kaolin (EPK)
2% cobalt carbonate
1 tin oxide

Very blue, bright, satinish and rather smooth. I've just tested it, so
I don't know all the particulars. It does not appear to move.

patrick conrey on mon 25 sep 00

Have you tried this glaze without the colorants???