search  current discussion  categories  glazes - cone 8-10 

tenmoku cone 10

updated wed 26 jul 00

 

Donald G. Goldsobel on tue 25 jul 00


Here is a favorite deep , translucent tenmoku that breaks to a rust on thin
and raised areas. It is Warren McKenzie's formula with some modification.
The kind of wood ash used has little effect if it is wood as opposed to
weeds etc. Good luck.
Mc Kenzie Tenmoku Modified Cone 10
WHITING 16
CUSTER 44
BALL 10
SILICA 22
WOOD ASH 7
FEO RED 9

Donald Goldsobel

>I am looking for glaze recipes for copperred (gerstley and non-gerstley) and
>tenmoku (reduction) that I can use as a starting point for experimentation.
>Cone 10 to 11, porcelain clay body.
>
>Thanks,
>Bruce
>
>___________________________________________________________________________
___
>Send postings to clayart@lsv.ceramics.org
>
>You may look at the archives for the list or change your subscription
>settings from http://www.ceramics.org/clayart/
>
>Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
>