Anderson Ranch Shino Slip

Soda Ash 3.2%
Spodumene 12.16%
Kona F4 8.64%
Neph Sy 36%
EPK 28%
OM4 Ball Clay 12%

I spray or dip the bone dry pots then bisque. I've only used this in
wood firing, haven't tried it in salt yet.