hal mc whinnie on wed 28 jun 00


-----Original Message-----
From: hal mc whinnie

Date: Wednesday, June 28, 2000 9:19 AM
Subject: glaze of week july 1 2000


>HAL'S SPODUMENE ONE
>CONE 9-10 REDUCTION
>high alumina matt glaze with little glaze flow
>dolomite 20
>custer 30
>epk 25
>whiting 5
>tin oxide 6
>bentonite 3
>total 89 grams
>add for colors
>iron oxide 5 yellow
>copper carb 2 blue green
>rutile 1 tan
>cobalt carb 3 black with all of above
>colors can be added as separate elements or combined
>for cone 7 substitute neph syn for custer
>to improve glaze flow add silica 10 grams
>
>this will produce the quintessential balanced glaze type which encourages
>reliable durable and non flowing glazes with appealing surface


these glazes will be kept as a separate book and will be offered in hard
copy beginning in the summer of 2001

these may be copied and stored by everyone on the listserv however all other
rights are reserved.
may not be published without permission

SEND ANY QUESTIONS TO AUTHOR AND DO NOT SEND TO THE LISTSERV