Hello All=21 Well, here's the first installment of my runny glazes =26 slips=
that
give the appearance of such. Please, I don't profess to the level of =
chemical
knowledge required to speak of food safety, so use at your own risk. My =
notes,
when I had written notes, are included. Also, if anyone else on list has
runny/textured glazes they'd like to share, please do, and I am also ALWAYS
looking for new oxidation tenmokus.

I will try my best to get the rest together later this coming week.



: ) Andie
----------------------------------------------------------------------------=
----


Slips by Phenomenal Philadelphia Ceramic Artist Candy DePew:
Base Formula:
Ingredient Amount

Ball Clay 25
Kaolin 25
Silica Flint 25
Nepheline Syenite 13
Gerstley Borate 12
=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F
For Colors Add:

Yellow: Rutile 15-20
Blue: Cobalt Oxide 2, Maganese Dioxide 2 (NOTE: under other blue glazes, =
this
gives a runny, denim textured appearance, even if layered under low-fire =
glazes)
Black: Red Iron Oxide 5, Maganese Dioxide 5
Green: Chrome Oxide 2

----------------------------------------------------------------------------=
----

Zakin=92s GK Drip Magic
Used to layer over other glazes to induce flow
=5E 6-7
Ingredient Amount

Frit 3124 18
Magnesium Carbonate 7
Neph Sye 10
Strontium 11
Spodumene 15
EPK 10
Whiting 13
Superpax 12
Unwashed Fireplace Ash 15
Bentonite 1

----------------------------------------------------------------------------=
----

Andie=92s Tiara
Micro-Crystalline Glaze
(NOTE: Transparent Grey/Blue Glaze with Small Dark Blue Crystals in Runs - =
DOES
RUN=21=21=21=21 Stilt well=21=21=21)
=5E7-8
Ingredient Amount
Custer Feldspar 154.38
Zinc Oxide 107.46
Dolomite 105.66
Lithium Carb 7.00
Red Iron Oxide 3.00

----------------------------------------------------------------------------=
----

IE 27: Green =26 Pink
(NOTE: if Copper carb upped to 2.5, becomes a cool lemongrass green that =
creates
a wonderful depth when layered, creates a glossy crackle when alone, does
pinhole some)
=5E 6

Ingredient Amount
Neph Sy 67
Dolomite 10
Kaolin 8
Silica Flint 9
Zinc Oxide 6
Red Iron Oxide 2
Copper Carb 1

----------------------------------------------------------------------------=
----



My version of a common Chappell Glaze (NOTE: layered, seems to make other =
glazes
run)
=5E 6-8
Ingredient Amount
Gerstley Borate 50.00
EPK 15.00
Silica 35.00
Frit =233134 15.00
Tin Oxide 5.00

----------------------------------------------------------------------------=
----

Ron Roy=92s Sapphire Revised
(NOTE: got this from Clayart - is a cone 6, but if fired to cone 7 or if =
refired
a second time to cone 6 it runs beautifully, and has great depth =26 =
texture.
Layers well, especially with browns and tans.)
=5E 6

Ingredient Amount
EPK 26
3134 37
Feldspar 16
Silica Flint 17
Strontium Carb 4
Rutile 4.5
Cobalt Carb 2.5
----------------------------------------------------------------------------=
----


Andie=92s Flowing Purple/Blue
(NOTE: glossy, very dark blues/purples, the higher fired the better the =
runs.)
=5E 6

Ingredient Amount
Feldspar 60
Whiting 10
Silica Flint 10
Gerstley Borate 10
Ball Clay 5
Kaolin 5
Bentonite 2
Manganese Dioxide 5
Cobalt Oxide 5

----------------------------------------------------------------------------=
----

Bahamas Blue
(NOTE: Runny, deeply textured blue/brown/white, one batch I mixed came out a
dark floating blue, must have messed up when mixing, usually a better color =
-
CHRIS SCHAFALE- this is the blue that was on the mug exchange mug I sent =
you. At
cone 7 or if refired to cone 6 a second time it runs very well. Stilt or be
ready to grind.)
=5E 6

Ingredient Amount
Neph Sy 470
Gerstley Borate 270
Flint 200
Kaolin 50
Red Iron Oxide 20
Cobalt Carb 15
Rutile 40

----------------------------------------------------------------------------=
----


Hope this keeps you guys busy until I can get back to the computer next week=
-
cross your fingers for tomorrow's show=21

: ) Andie