Raku Glaze
==========
FRIT 6004........... 70.00 70.00%
WOLLASTONITE........ 30.00 30.00%
========
100.00

CaO 0.51* 14.48%
K2O 0.23* 10.85%
Na2O 0.26* 8.05%
Al2O3 0.05 2.45%
B2O3 0.51 17.85%
SiO2 1.53 46.32%

Si:Al 32.10
SiB:Al 42.78
Expan 11.18

Notes:
Apply thick for larg crakles( from Yehuda Koren)
==================================

Frit 6004
=========
Na2O................ 11.50 11.50%
K2O................. 3.50 3.50%
K2O................. 15.50 15.50%
Si2O3............... 44.00 44.00%
B2O3................ 25.50 25.50%
========
100.00
=============================
FRIT F-15
=========
K2O................. 3.60 3.60%
Na2O................ 2.60 2.60%
B2O3................ 23.00 23.00%
Al2O3............... 3.81 3.81%
SiO2................ 67.00 66.99%
========
100.01