Dave Finkelnburg on thu 16 mar 00

-------------------
I am testing some Laguna Cone 10 B-Mix. Would someone be willing to share a
clear glaze recipe which they have found has good =22fit=22 on this clay at =
Cone 10?
I'd like to use the recipe as a basis for getting the expansion value right,=
or
pretty close, early in this testing process. Thanks in advance for any =
help=21
Dave Finkelnburg
dfinklen=40cyberhighway.net

Don Prey on fri 17 mar 00

------------------

In a message dated 3/16/2000 6:46:43 PM, dfinkeln=40cyberhighway.net writes:

=3C=3C I am testing some Laguna Cone 10 B-Mix. Would someone be willing to =
share
a

clear glaze recipe which they have found has good =22fit=22 on this clay at =
Cone
10?

I'd like to use the recipe as a basis for getting the expansion value right,
or

pretty close, early in this testing process. Thanks in advance for any =
help=21

Dave Finkelnburg =3E=3E

Dave, the following would be my best recommendation for a starting point:

Glaze name: EB CELEDON BASE
Cone: 9 - 11
Color:
Testing: tested
Surface texture: shiny glossy
Firing: Ox. or Red.
Glaze type:

Recipe: Percent Batch
FLINT 39.10 39.10
WHITING 17.87 17.87
CUSTER FELDSPAR 24.83 24.83
EPK 18.20 18.20
Totals: 100.00 =25 100.00 gm

Comments:
FOR USE WITH B-MIX. NO CRAZING.
green: 0.8 green chrom =26 3.0 rutile.

Possible Health Hazards:
Flint: free silica-wear a NIOSH approved dust mask when handling dry =
material


Unity Formula for EB CELEDON BASE:
0.126 K2O=A0 0.491 Al2O3 4.856 SiO2=A0
0.054 Na2O 0.005 Fe2O3 0.005 TiO2=A0
0.815 CaO=A0 9.9:1 Si:Al Ratio
0.005 MgO=A0

Percentage Analysis:
72.20 =25 SiO2
12.40 =25 Al2O3
2.95 =25 K2O
0.82 =25 Na2O
11.31 =25 CaO
0.05 =25 MgO
0.20 =25 Fe2O3
0.10 =25 TiO2

Don Prey in Oregon