search  current discussion  categories  glazes - misc 

missing recipe-help (all is revealed)

updated thu 3 feb 00

 

Don Goodrich on wed 2 feb 00

Hi Jim,
Hard drives are our compensation for senior moments ;) The recipe you
have is from a post a couple of years ago by Norm Straker, who appears to no
longer be on this list.
Here, from my hoard, are the relevant Clayart posts:

-----------------------------

>Date: Thu, 4 Dec 1997 08:06:37 EST
>From: Norm
>Subject: Cranberry or Blood red!
>
>----------------------------Original message----------------------------
>Hey Folks,
>
>I am looking for a glaze batch that will produce a Cranberry or Blood
>red at cone 6 oxidation. Any favorites??
>
>Thanks, Norm
>
>------------------------------
>
>Date: Fri, 13 Feb 1998 09:24:22 EST
>From: Norm
>Subject: Cone 6 glaze - ox blood red
>
>----------------------------Original message----------------------------
>Hey folks,
>
>This one I got from Clayart. Just fired it and I love it. Seems to
>come out best on white claybody.
>
>APPLY HEAVILY FOR BEST RESULTS
>GERSTLEY BORATE 54.88
>TALC 14.63
>FLINT 30.49
>
>ADD RED IRON OXIDE 21.95%
>
>FROM ANDREW S. LUBOW (CLAYART 9-28-96)
>
>Norm! 8^o
>====================

Hope this helps solve the mystery.

Don Goodrich in Zion, Illinois and tired of snow
goodrichdn@aol.com