Bubbly Grey
This is a cone 9-10 glaze recipe I have from Bennington.

Custer spar 75
Ball clay 5
Ash 12
Neph. Sye. 8

It is a smooth glaze with bubbles under the surface, shiny, not much color. =
I
have not used it in more years than I care to remember, but I recall liking =
it a
lot.