Carolyn- sorry, deleted your address so will reply here. For
Standard's 182 white stoneware, a good clear is the one in CM 10/95,
from Chartrand and Sodersten. I fire at ^8-9. This glaze is billed as
^7-9. Doesn't craze.

CLEAR GLAZE

Gerstley borate 21

wollastonite 8

neph sy 30

Kentucky ball clay 10

flint 31

Mimi in NJ